ylz301 --- 2015-01-30 20:42:55
1
擠出PVC的外護(hù)套,用擠壓式擠出,護(hù)套厚1.2mm,擠出的表面現(xiàn)纜芯包帶的節(jié)距,為什么?
fmy051424 --- 2015-02-02 10:46:29
2
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:14
3
鎧裝鋼帶不夠平整,護(hù)套基礎(chǔ)溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:16
4
鎧裝鋼帶不夠平整,護(hù)套基礎(chǔ)溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:22
5
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:25
6
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:26
7
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:27
8
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:28
9
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:29
10
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:30
11
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:30
12
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
fmy051424 --- 2015-02-02 11:04:30
13
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
ydk777 --- 2015-02-02 11:45:19
14
要看你是多大的線,內(nèi)模退遠(yuǎn)點(diǎn)試試,不行再近點(diǎn)看看,還有就是內(nèi)絞合是不是規(guī)則
xushuyong --- 2015-02-02 16:10:36
15
頂~~~~~~~~~~~~~~~~~~~~
ylz301 --- 2015-02-02 20:22:30
16
纜芯圓整,纜芯最外層包的聚酯帶,護(hù)套外顯聚酯帶的包帶搭接部分的節(jié)距痕跡。
578578 --- 2015-02-04 10:16:27
17
壓力過(guò)大,或者外模選擇不當(dāng)
ZJM809218 --- 2015-02-04 14:40:40
18
ydk777:
要看你是多大的線,內(nèi)模退遠(yuǎn)點(diǎn)試試,不行再近點(diǎn)看看,還有就是內(nèi)絞合是不是規(guī)則
同意
ZJM809218 --- 2015-02-04 14:41:40
19
2~13樓奇葩一個(gè),沒(méi)有見(jiàn)過(guò)鋼帶鎧裝的還直接擠壓式護(hù)套的
zh022 --- 2015-02-04 15:09:32
20
你說(shuō)的其實(shí)是一個(gè)人
736037161 --- 2015-02-05 15:43:25
21
鎧裝鋼帶不夠平整,護(hù)套擠出溫度偏高,拉伸比偏大
遺忘的石像 --- 2015-02-06 07:59:05
22
頂~~~~~~~~~~~~~~~~~~~~
jolinchen --- 2015-02-06 14:28:35
23
樓主問(wèn)的問(wèn)題就有問(wèn)題,除了告知外被材質(zhì)為PVC,擠出方式,皮厚為1.2mm,其它什麼信息都沒(méi)有,叫別人怎麼給你分析?
你要告知是什麼線?線內(nèi)結(jié)構(gòu)是怎樣的?線徑多大?這些基本的信息,這樣才利於給人分析呀。
luo1984 --- 2016-06-17 05:20:29
24
能否把聚酯帶改為無(wú)防布,(因?yàn)榫埘П容^硬);蛘咦o(hù)套料改硬點(diǎn)。不然就是做出來(lái)了,在打卷時(shí)也有明顯節(jié)距痕跡。